Metric Bolt, Screw and Nut Strength — ISO 898 Property Classes

ISO 898-1 property classes 3.6 to 12.9 — nominal and minimum tensile strength, lower yield and 0.2% proof stress — plus ISO 898-2 nut-to-bolt class pairing and the ISO 3506 stainless groups and grades with their minimum strengths.

Last updated: 2026-11

Request a Quote

Metric Bolt, Screw and Nut Strength — ISO 898 Property Classes in an industrial setting
Illustrative image redrawn from real Metric Bolt, Screw and Nut Strength — ISO 898 Property Classes product references — not a photograph of stocked items.

Specifications

The property class stamped on a metric bolt or screw is its strength certificate in two numbers: the first digit is 1/100 of the nominal tensile strength in kgf/mm 2 tradition, the second is roughly the ratio of yield (or proof) to tensile. This reference collects the strength tables behind that system in one page. The ISO 898 table covers classes 3.6 through 12.9: nominal tensile from 300 (class 3.6) to 1200 (class 12.9), minimum tensile, and — split by hardening route — lower yield strength R eL,min for the ductile classes 3.6-6.8 (e.g. 4.6: 240) versus 0.2% non-proportional elongation stress R p0.2,min for the hardened classes 8.8 up (e.g. 12.9: 1100). Class 8.8 is split by diameter: up to 16 mm it prints 800/640, above 16 mm 830/660 — the same marking, two strength rows. The ISO 898-2 pairing table follows: a class-8 nut mates up to class 8.8 bolts, a class-10 nut up to 10.9, and so on. The ISO 3506 stainless tables close the page: the austenitic (A1-A5), martensitic (C1/C3/C4) and ferritic (F1) groups, and the grade/class grid with minimum tensile and 0.2% proof stress — A2-70: 700/450, A4-80: 800/600, C1-110: 1100/820. Use it to decode markings, check a pairing, or compare a carbon-steel class against a stainless grade at quotation. Proof loads, test mandates and marking rules are per RFQ against the standards themselves.

Carbon/n alloy steel classes 3.6, 4.6, 4.8, 5.6, 5.8, 6.8, 8.8 (d <= 16 and d > 16), 9.8, 10.9, 12.9 — nominal tensile 300-1200, min tensile 330-1220
Yield vs proof columns Classes 3.6-6.8: lower yield R eL,min (180-480); 8.8 and above: 0.2% proof R p0.2,min (640-1100); en-dash cells mark not-tabulated values as printed
Nut pairing Nut class 5 -> bolts up to 5.8; 6 -> 6.8; 8 -> 8.8; 10 -> 10.9; 12 -> 12.9 (where permitted by ISO 898-2)
Stainless groups Austenitic A1/A2/A3/A4/A5, martensitic C1/C3/C4, ferritic F1 per ISO 3506
Stainless grade strengths Austenitic 50/70/80/100: 500/700/800/1000 min tensile with 210/450/600/750 proof; C1 up to 110 (1100/820); C3-80 (800/640); F1-45 and -60 (450/250, 600/410)
Not tabulated Hardness ranges, proof loads in kN, test frequencies, marking layout, temperature limits — per RFQ
Metric bolt, screw and nut strength — ISO 898 property classes (3.6 - 12.9)As printed on the collected page: nominal and minimum tensile strength, lower yield strength and 0.2% non-proportional elongation stress per property class. Subscripted strength symbols carry the corpus's spaced form (R m,nom, R eL,min, R p0.2,min) reproducing the page's sub/italic markup; the live page prints them collapsed (Rm,nom). The en-dash cells mark values the source does not tabulate. Verification: re-fetched from the live page 2026-11-01, all 12 rows equal to the x127 corpus (2 header rows equal modulo the documented markup-spacing convention).
Property ClassNominal Tensile Strength R m,nomMinimum Tensile Strength R m,minLower Yield Strength R eL,min0.2% Non-Proportional Elongation Stress R p0.2,min
3.6300330180–
4.6400400240–
4.8400420320–
5.6500500300–
5.8500520400–
6.8600600480–
8.8 – d ≤ 16 mm800800–640
8.8 – d > 16 mm800830–660
9.8900900–720
10.910001040–940
12.912001220–1100
  • Row 1 (3.6): classes 3.6-6.8 carry lower yield strength R eL,min; 8.8 and above carry 0.2% proof R p0.2,min (hardened classes have no distinct yield plateau) — the en-dash cells are the source's own not-tabulated markers
  • Row 7 (8.8 – d ≤ 16 mm): class 8.8 is split by diameter (d <= 16 mm vs d > 16 mm) with different R m,min and R p0.2,min — as printed
Nut property class vs typical mating bolt property classAs printed on the collected page, pairing nut classes to the bolt classes they are rated to mate with under ISO 898-2. Verification: re-fetched from the live page 2026-11-01, all 6 rows token-for-token equal to the x127 corpus.
Nut Property ClassTypical Mating Bolt Property Class
5Up to property class 5.8 where permitted by ISO 898-2
6Up to property class 6.8 where permitted by ISO 898-2
8Up to property class 8.8 where permitted by ISO 898-2
10Up to property class 10.9 where permitted by ISO 898-2
12Up to property class 12.9 where permitted by ISO 898-2
Stainless steel fastener groups per ISO 3506As printed on the collected page: the ISO 3506 stainless groups with their designations and general descriptions, carried verbatim. Verification: re-fetched from the live page 2026-11-01, all 4 rows token-for-token equal to the x127 corpus.
GroupDesignationGeneral Description
AusteniticA1, A2, A3, A4, A5Chromium-nickel and chromium-nickel-molybdenum stainless steels widely used where corrosion resistance is required. Austenitic grades are generally non-magnetic in the solution-annealed condition but can become partly magnetic after cold working.
MartensiticC1, C3, C4Hardenable stainless steels capable of relatively high mechanical strength. Their corrosion resistance is generally lower than that of common austenitic stainless steels.
FerriticF1Chromium stainless steels with magnetic behaviour and mechanical and corrosion properties differing from the austenitic grades.
Stainless steel grades — minimum tensile and 0.2% proof stress (ISO 3506)As printed on the collected page: minimum tensile strength and minimum 0.2% proof stress in N/mm 2 per stainless group, grade/type and property class. Subscripted symbols carry the corpus's spaced form (R m, R p0.2). Empty leading cells mark continuation rows of the preceding group — as printed. Verification: re-fetched from the live page 2026-11-01, all 11 rows equal to the x127 corpus (colspan-expanded live grid).
Stainless GroupGrade / TypeProperty ClassMinimum Tensile Strength R m (N/mm 2 )Minimum 0.2% Proof Stress R p0.2 (N/mm 2 )
AusteniticA1, A2, A3, A4, A550500210
70700450
80800600
1001000750
MartensiticC1 / C450500250
C1 / C470700410
C11101100820
MartensiticC380800640
FerriticF145450250
60600410

Materials

  • The tenant supplies fasteners across these classes — carbon and alloy steel property classes, and stainless to the A2/A4 austenitic grades that dominate industrial demand (the A1-A5/C/F designations on this page map to those supply grades). State the property class or stainless grade, the size, and any certificate requirement (EN 10204 3.1) on the RFQ; strength values are delivered against the standard and the certificate, and class pairings (bolt + nut) are honoured as specified

Ordering & documentation

Documents

Shipments of Metric Bolt, Screw and Nut Strength — ISO 898 Property Classes are backed by Mill Test Certificate (MTC), Dimensional Report, Salt Spray Test Report on request, with full batch traceability from raw material to finished product. Quality management for Metric Bolt, Screw and Nut Strength — ISO 898 Property Classes orders follows the owner-confirmed compliance list: ISO 9001:2015, RoHS, REACH. Exact document sets are confirmed on the order.

Quotation

  • The product family (Metric Bolt, Screw and Nut Strength — ISO 898 Property Classes), product standard/designation and drawing or part number.
  • The dimensions that apply to this part — such as size, pitch, length, thickness, fit, grip or groove geometry.
  • Material/grade, heat-treatment condition and surface finish, together with the service environment.
  • Quantity per size, delivery destination and required test or traceability documents.

Sample & supply

Minimum order quantity for metric bolt, screw and nut strength — iso 898 property classes is 10,000 pieces (applies to the standard sizes and finishes for metric bolt, screw and nut strength — iso 898 property classes; mixed, special or custom variants are quoted — final commercial terms per quotation) Stock items for metric bolt, screw and nut strength — iso 898 property classes run 3–7 days. Quantities or variants of metric bolt, screw and nut strength — iso 898 property classes outside the standard range are confirmed at quotation.

Storage & shipping

Metric Bolt, Screw and Nut Strength — ISO 898 Property Classes are packed for export and shipped factory-direct to buyers in Europe, Asia, the Americas and the Middle East. Store metric bolt, screw and nut strength — iso 898 property classes dry and protected until installation, and keep coated parts in their packaging until use; specific packing and preservation requirements can be stated on the order and confirmed at quotation.

Frequently asked questions

How do I read a property-class marking like 8.8 or 10.9 into actual strength numbers?

Use the two digits as a shorthand and this page's table as the exact values. For 8.8: the 8 signals a nominal tensile strength of 800 (units as tabulated) and the .8 that yield/proof is 0.8 times that — check the table row and you find proof 640 for sizes up to 16 mm. For 10.9: nominal 1000, proof at 0.9 of it = 900... the table prints 940, because the standard rounds the relationship per class rather than deriving it — this is exactly why you read the table instead of computing. One trap the table makes visible: class 8.8 has two rows (d <= 16 mm: 800/640; d > 16 mm: 830/660), so a big M 24 "8.8" bolt is actually held to a higher minimum than an M 10 one. And the yield/proof column switches meaning at 8.8 — ductile classes report lower yield, hardened classes report 0.2% proof, because hardened steel has no flat yield plateau.

Does a class-10 nut on a class-8.8 bolt work, and what does the stainless A2-70 marking mean?

Yes — and it is deliberate. The pairing table says a class-10 nut mates bolts up to class 10.9, so class-10 on an 8.8 bolt is a valid, slightly over-strong nut choice; the reverse (an 8 nut on a 10.9 bolt) is not, because the nut threads would strip before the bolt reached its strength. Over-specifying the nut is the cheap insurance most joint designers accept. For stainless: A2-70 decodes as austenitic grade (A2 is the common 304-family), property class 70 — the 70 is 1/10 of the minimum tensile strength, 700, with 0.2% proof 450 from this page's table. The same grade can come as A2-50 (soft, 500/210) or A2-80 (800/600, cold-worked), which is why "A2" alone is not a strength statement — always quote grade plus class (A2-70, A4-80) on the RFQ so the certificate matches the marking.

What is the MOQ and lead time for Metric Bolt, Screw and Nut Strength — ISO 898 Property Classes?

Orders under this designation have a minimum order quantity of 10,000 pieces. Stock items ship in 3–7 days. Final commercial terms are confirmed per quotation.

What should an RFQ for Metric Bolt, Screw and Nut Strength — ISO 898 Property Classes state?

State the full designation (Metric Bolt, Screw and Nut Strength — ISO 898 Property Classes), thread size and pitch or diameter, length or head dimension, finish, quantity per size, plus the destination country and any required certificate such as a mill test report per EN 10204 3.1; dimensions and schedule for this designation are confirmed with the quotation.

Request a Quote

Get factory-direct pricing from the manufacturer.

What to include in your Metric Bolt, Screw and Nut Strength — ISO 898 Property Classes inquiry

  • ✓ Identify the screw type and standard, including head style and drive recess.
  • ✓ Give nominal diameter, thread pitch, length and engagement or hole details where relevant.
  • ✓ State the material/property class, substrate material and thickness, and required coating or finish.
  • ✓ Describe installation, locking or removal requirements, quantity and destination.
  • ✓ Factory-direct pricing for your Metric Bolt, Screw and Nut Strength — ISO 898 Property Classes
  • ✓ Standard and custom specifications
  • ✓ Factory-direct export to buyers in Europe, Asia, the Americas and the Middle East
  • ✓ Full fastener family support